Laser Cut Dross: Why the Bottom Edge Grows a Burr
Laser cut dross forms when melt freezes before the assist gas clears the kerf. What the shape of the burr tells you, and how to spec the edge on a drawing.
Flip a laser-cut part over and run a finger along the bottom edge. Clean on top, sharp underneath is the usual complaint, and laser cut dross is what you're feeling. It's not random, and the shape of it says a lot about where it came from.
Why Is There a Burr Hanging Off the Bottom of a Laser-Cut Part?
Molten metal froze before the assist gas could blow it out of the kerf. Gas pressure at the head, focus position, cutting speed and heat buildup cause it far more often than a worn nozzle does.
Hard Metal Explained makes that case in Bottom-Edge Burr On Laser Parts: Why A New Nozzle Won't Fix It. Nitrogen-cut stainless needs a lot of gas to push melt out the bottom, often well over 10 bar, and the tank gauge can read fine while pressure at the head sags on thick work. Set the focus too high on stainless and the cut narrows toward the bottom, so the gas can't get in. A nozzle only matters, the video says, when it's actually dented or crusted with spatter.
Slower Isn't Cleaner
The instinct is to slow down. Charles Caristan of Air Liquide told The Fabricator that this often makes the burr bigger. Too slow puts extra heat in the kerf. The vapor from that extra heat disturbs the gas flow, and the metal it fails to clear freezes into what the article describes as a stalactite on the bottom edge. Sometimes the fix is a slightly faster feed.
Reading Laser Cut Dross on Your Parts
The video gives a decent field guide. Loose round droplets that knock off easily usually mean too much heat. A hard, sharp beard stuck to the edge means the gas isn't reaching the bottom. Burr on one side only points to a beam that's off center in the nozzle, and burr that creeps in over a shift usually means a dirty protective window.
Two patterns are worth knowing as a designer. Burr that shows up only in corners and small holes comes from the head slowing down while power stays high, and modern controls ramp power down to match. On thick mild steel cut with oxygen, the last parts off a tightly packed sheet can drag dross because the plate has soaked up heat. Thicker stock also runs rougher toward the bottom of the cut anyway, as why laser cutting leaves a tapered edge explains, and gas choice on stainless is its own topic in nitrogen vs oxygen.
Putting It on the Drawing
If the bottom edge touches a hand or a mating part, say so. A clear edge note beats hoping, and break all sharp edges covers how to word one.
Our sheet metal work is laser cut to ±0.13 mm in Cold Rolled Steel, Stainless 304 and the other stock sheets. Deburring isn't listed on that page, so if an edge has to be burr-free, ask us when you quote.
Need a part made?
Upload your file for an instant price.