SLS doesn't need supports, so it's easy to assume it doesn't care which way a part sits in the powder. SLS part orientation still changes how the part looks and how its holes fit. Strength moves a little too, just not much.

Does Part Orientation Matter in SLS Printing?

Yes, mostly for surface and detail. Faces printed pointing up come out smoother and crisper than faces pointing down, while strength changes far less than it would on a filament printer.

Everything SLS tested this in Part Orientation: How Does it Impact Your Part, on an SLS4ALL Inova MK1 desktop machine. The description says it "compares the difference in parts with features that are printed face down versus face up." He printed the same test plate both ways, then measured and compared them.

What the Face-Up vs Face-Down Test Showed

Face up, the raised letters and numbers were sharp and the top surface was smooth. The side that printed face down came out grainier, and its lettering was rounder and softer. Hubs' guide to build orientation says the same about powder-bed parts in general: "lower surfaces typically exhibit a grainier finish."

Dimensions shifted as well. On the face-up plate the outside diameters landed very close to nominal. Face down, the posts ran about 0.1 mm small. Holes came out undersized either way, by a bit under 0.3 mm, which he ties to the roughly 0.3 mm gap he finds SLS can reliably hold. That's one desktop machine and one test part, so take the direction, not the numbers.

Strength barely moved. His flat tensile bars averaged about 42 MPa, and one bar from an earlier build that sat slightly tilted toward Z tested about 5 to 6% weaker. Hubs describes SLS and MJF parts as "effectively isotropic," and a single-digit gap fits that.

Using SLS Part Orientation on Your Own Parts

Decide which face is cosmetic and which features carry fine detail, like printed text or a snap catch. Those are the ones you'd want facing up.

Holes and pins that have to mate need some extra room, since powder-printed holes tend to come out small. Print-in-place clearance for SLS and MJF has numbers for moving parts. Sealing walls care about orientation for a different reason, covered in watertight MJF parts. If you're still choosing a process, see MJF vs SLS for a functional nylon part.

Our 3D printing runs industrial SLS and MJF at ±0.3 mm or ±0.3%, whichever is greater. If a cosmetic face or a fine feature needs to point up in the build, ask us when you quote.