← All posts

Galvanic Corrosion: Stainless Screws in Aluminum Parts

Galvanic corrosion eats the aluminum around a stainless screw, but only while the joint is wet. When it matters on a machined part and how to isolate it.

Plenty of aluminum housings get bolted together with stainless hardware, and sooner or later someone asks whether that's a mistake. Galvanic corrosion is real, but it needs water to run, and on most indoor parts it never gets any.

Stainless Bolt in Aluminum: Which One Corrodes, and How Fast?

The aluminum corrodes and the stainless screw is protected. How fast depends on how often the joint is wet and how salty the water is. In dry inland air the effect is negligible.

That's the answer Solaracks gives in Stainless Bolt, Aluminium Rail: Who Corrodes?, a video about anodized aluminum solar racking held together with stainless bolts. The attack only works while a water film wets both metals, and it stays within a few millimetres of the contact. The video cites University of Hawaii tests where the galvanic current from 316L made up only about 5 to 15% of the aluminum's total corrosion. Where salt water sits on a joint, it says modelling puts local loss at up to 0.1 mm a year, and around 1 mm a year in a narrow crevice.

Why Area Ratio Decides Galvanic Corrosion

A small stainless screw in a big aluminum part spreads the attack over a lot of metal. Flip it and you're in trouble. The ASSDA technical FAQ says aluminum fasteners in stainless aren't acceptable, while a stainless screw in aluminum is common practice even though the aluminum right around it can still go. Their rule of thumb: once the corroding metal's wetted area is ten times the noble metal's, galvanic effects aren't serious.

There's a catch they point out. As a joint dries after rain, the wet area shrinks toward the crevice under the head, so a ratio that looked like 1:50 can end up close to 1:1.

Anodize Doesn't Cover the Threads

The anodic film is an insulator, so a screw head sitting on intact anodize isn't touching aluminum. The threads are another story. The Solaracks parts were anodized before they were drilled and tapped, which left bare aluminum in every hole, and that's where the white powder shows up first. Chem film behaves differently because it stays conductive; chem film vs anodize covers that tradeoff.

ASSDA is blunt that paint isn't a dependable insulator under a bolt head. Plastic washers and sleeves are what actually break the circuit.

What We'd Do on a Machined Part

Indoors, Stainless 304 screws in Aluminum 6061 are normal and we wouldn't worry. Near the coast, isolate the joint or seal it, and think about 316 vs 304 for the hardware itself. If the stainless part is one we machine, passivation is a separate question worth reading.

Our CNC quote costs every tapped hole as its own feature. If you need the part anodized after tapping, or isolating hardware supplied, ask us when you quote.

Need a part made?

Upload your file for an instant price.

Start a quote